Drains
Yeah, nah.
- Messages
- 7,718
- Location
- Sefton, South Island, NZ
As above- arc weld with ni or ni/fe rods, take off the chill but never weld more than about 15mm at a time, don't continue until the weld is cool enough to touch. If you're not patient, it will crack (and you'll hear that "ting" when it goes). Take your time and it'll work.